image
image
user-login
Patent search/

LOCALISED WHITENING OF JUTE TO CREATE VALUE-ADDED TEXTILES

Patent Search in India

  • tick

    Extensive patent search conducted by a registered patent agent

  • tick

    Patent search done by experts in under 48hrs

₹999

₹399

Talk to expert

LOCALISED WHITENING OF JUTE TO CREATE VALUE-ADDED TEXTILES

ORDINARY APPLICATION

Published

date

Filed on 22 April 2024

Abstract

Abstract LOCALISED WHITENING OF JUTE TO CREATE VALUE-ADDED TEXTILES Jute, the golden fibre is traditionally used mostly as packaging material and to make sacks and coarse fabric. The jute industries are paying less attention to innovative designs and applications of jute fibres in various fields. Hence, there is a serious need to use jute in diverse fields through design innovation. In the present invention, jute yarns are selectively bleached through an eco-friendly bleaching process as per the design, followed by weaving in handloom that creates special design effects in the ultimate fabric. In this method, jute yarns are treated with 10% (w/v) sodium hydroxide at room temperature for 45 minutes which swells the fibre along with the development of crimp, followed by neutralization with 2% acetic acid solution. The alkali-treated jute yarns are placed in the creel and then tied using plastic sheets to impede the bleaching agent from going inside the tied areas. These partially bleached jute yarns are used as weft and create an Ikkat-like effect when woven in the handloom. This fabric is then used for producing jacket (Figure 7).

Patent Information

Application ID202431031716
Invention FieldTEXTILE
Date of Application22/04/2024
Publication Number18/2024

Inventors

NameAddressCountryNationality
Dr. Sankar Roy MaulikDepartment of Silpa-Sadana, Visva-Bharati (A Central University) P.O. Sriniketan District: Birbhum, West BengalIndiaIndia
Shri Ritwick HalderDepartment of Silpa-Sadana, Visva-Bharati (A Central University) P.O. Sriniketan - District: Birbhum, West BengalIndiaIndia

Applicants

NameAddressCountryNationality
Dr. Sankar Roy MaulikDepartment of Silpa-Sadana, Visva-Bharati (A Central University) P.O. Sriniketan District: Birbhum, West BengalIndiaIndia
Shri Ritwick HalderDepartment of Silpa-Sadana, Visva-Bharati (A Central University) P.O. Sriniketan - District: Birbhum, West BengalIndiaIndia

Specification

Description:FORM 2
The Patents Act, 1970
(39 of 1970)
&
The Patents Rules, 2003
COMPLETE SPECIFICATION
(Section 10 and Rule 13)


Title Of The Invention
"LOCALISED WHITENING OF JUTE TO CREATE VALUE-ADDED TEXTILES"

APPLICANT
Name (1): Dr. Sankar Roy Maulik
Name (2): Shri Ritwick Halder
Nationality (1 & 2): INDIAN
Address (1 & 2): Department of Silpa-Sadana,
Visva-Bharati
(A Central University)
P.O. Sriniketan - 731236
District: Birbhum, West Bengal

The following specification particularly describes the invention and
the manner in which it is to be performed


LOCALISED WHITENING OF JUTE TO CREATE VALUE-ADDED TEXTILES



Field of Invention

The present invention relates to localised whitening of jute to create value- added textiles with resisting effect. More particularly, this invention relates to alkali-treated jute yarns followed by resist bleaching to obtain partially whitened jute to produce aesthetically pleasing value-added apparel (jacket). Background Art
The extensive use of synthetic materials has resulted in a higher level of pollution and thus is proving detrimental effect to both the environment and living organisms. Thus, it is critically necessary to replace synthetic materials with natural, renewable, and biodegradable ones from a sustainability perspective. Recently, jute has been recognised as one of the most sustainable and economical natural resources with varied uses. Jute, in turn, adds up to the country's circular economy. In addition to the various beneficial attributes, jute fibre has certain mechanical and chemical limitations that hinder its use in various fields. This work primarily discusses how these limitations can be aesthetically designed to create products of varied utility, thus proposing a completely new technique to add value using this limitation. Photo yellowing is one of the major disadvantages of jute fibre. It refers to the process by which fibres get discoloured and turned into yellow when exposed to light. This is a common problem with jute fibres and can occur when the fibres are exposed to UV light or other forms of light over an extended period. This phenomenon has been thoroughly observed and studied to create an aesthetic effect through selective whitening using the resist beaching technique. The resist technique is popularly used in dyeing, but the aesthetic effect through resist bleaching is not available in the literature. In this process, the effect of photo yellowing can be checked and converted into design effects. Detailed research and experiments have been carried out to ensure its application as clothing as well as furnishing material.
In the prior art, a PCT application WO2022157728A1 discloses a treated fabric for grain storage includes plural jute fibres woven together to form a fabric, the plural jute fibres having a smooth external surface; first rough

regions formed into the external surface of a jute fibre of the plural jute fibres; second rough regions formed into the external surface of the jute fibre; and a paraffin wax layer located over the external surface of the jute fibre, the first rough regions, and the second rough regions. The first rough regions originate from a different substance than the second rough region, and the second rough region is deeper than the first rough region.
In another prior art, an US specification US3521991A discloses a process for improving the lightfastness of jute and removing surface hairiness which comprises a first step of contacting jute with a material selected from the group consisting of 1) moist chlorine gas, (2) an aqueous chlorine solution and (3) an aqueous solution of hypochlorous acid, the period of contact for (l) and (2) being about 2 to 10 minutes and the period of contact for 3) being about 5 to 15 minutes, said aqueous solution of hypochlorous acid having a pH of about 6 and containing about 5-10% available chlorine based on the weight of the jute; and a second step of extracting the so-treated jute with an aqueous solution of at least one compound selected from the group consisting of sodium and potassium hydroxides, phosphates, sulphites and bisulphites for a period of about 5 to 20 minutes, the solution or sodium or potassium sulphite containing about 2.5 to 10% of sodium or potassium sulphite based on the weight of the jute and the remaining compounds being present in solution in an amount of about 5-10% based on the weight of the jute.
In yet another prior art a US application US534450 discloses a process of bleaching and decolouring fibres and the like which consists of treating the same in a bath containing a substance having a protective action on the fibres, such as a sulfonated or soluble oil; then in a bath containing a manganate, or permanganate salt; then in a bath having a bleaching or whitening action; and then washing.


Summary of Invention

A process for localised whitening of jute through bleaching to create value- added textiles wherein jute yarns are subjected to swelling agents by treating with 10% (w/v) sodium hydroxide (NaOH) at room temperature for
45 minutes, followed by washing. This phenomenon causes differential

shrinkage of the matrix and the ultimate cells of the fibre. This causes the darkening of jute which is an utmost undesirable condition. In this invention, this darkening has been utilised to add prominence to the effect. The alkali-treated jute yarns are placed in creel as per the loom specifications and then tied using plastic sheets to prevent the bleaching agent from going inside the tied portions followed by washing in cold water and sun-drying. The bleaching process is done with 30% (w/v) hydrogen peroxide (6%), sodium silicate (3%), tri-sodium phosphate (2%), sodium carbonate (2%), and detergent (0.5%) at a temperature of 85O C for 2 hours keeping material to liquor ratio 1:30 at pH 10.5-11 followed by hot wash (70OC) and cold wash.


Brief Description of the Accompanying Drawings

Figure 1 illustrates alkali-treated jute yarn in accordance with the present invention;
Figure 2 illustrates the tying of alkali-treated jute yarn with plastic sheets and nylon threads in accordance with the present invention;
Figure 3 illustrates bleaching of tied jute yarn with hydrogen peroxide in accordance with the present invention;
Figure 4 illustrates the removal of threads and plastics after bleaching in accordance with the present invention;
Figure 5 illustrates partially bleached jute yarn in accordance with the present invention;
Figure 6 illustrates handloom weaving product in accordance with the present invention;
Figure 7 illustrates a diversified jute product (Jacket) in accordance with the present invention.


Detailed Description

Bleaching of jute is a process used to remove the natural pigments and other impurities from jute fibres, making them lighter in colour and more suitable for various applications. Bleaching improves aesthetic appearance and dyeing characteristics of jute fibre, allowing it to be used in a wider range of products.

In this study, the jute yarns are subjected to selective bleaching as per the design and then woven in the loom, creating special design effects in the resultant fabric. The bleaching is primarily carried out using common bleaching agents i.e., hydrogen peroxide. Bleaching of jute is one of the tedious processes and can lead to patchy and ineffective bleaching if not done carefully. In the present work, this localised bleaching process was used from the design perspective to create a distinct effect on woven fabric. This style of resist bleaching of weft jute yarns resembles the fabrics produced with traditional Ikkat, which is a traditional dyeing technique used to create intricate patterns and designs of woven fabric.
Jute, the golden fibre is an important natural fibre primarily grown in India and Bangladesh. It is long, strong, and durable, which makes it ideal for manufacturing a range of products, including bags, ropes, carpets, and other textiles. Jute products have also played an important role in the country's economy and have created many employment possibilities. Jute may be grown with low amounts of pesticides and fertilizer. Jute plants purify the air by consuming vast volumes of carbon dioxide, the primary cause of the greenhouse effect. It lowers carbon footprint as well. During the
100-day growing season, one hectare of jute plants may absorb 15 tonnes of carbon dioxide from the atmosphere and release 11 tonnes of oxygen. Less energy is required to produce one tonne of jute fibre than one tonne of synthetic counterpart. Jute can be continually cultivated and harvested with a small amount of water. It replenishes soil nutrients and decreases pest risk. Jute has excellent insulating and antistatic qualities, low thermal conductivity, and moderate moisture retention. Besides these attributes, it promotes craft clusters and industrial productions at a similar pace. These unique characteristic properties of this 'golden fibre' have generated interest in studying and understanding this fibre and its disadvantages so that it can be used in value-added products and introduce new interventions in all the craft clusters working with jute as the primary material.
In this process, the jute yarns were initially subjected to swelling agents i.e., treated with 10% (w/v) sodium hydroxide (NaOH) at room temperature for
45 minutes, followed by neutralisation with 2% acetic acid solution. During this process, the hemicellulose is removed and crimps are developed, thus

making it much softer than the raw fibres. The major drawback of this alkali treatment is that it turns the fibre dark; however, in the resisting process, this darkness adds to the prominence of the designs. After treatment with the swelling agent, the yarns were placed in creel following the loom specifications and then tied using plastic sheets to prevent the bleaching agent from entering the tied portions. After bleaching the yarns were washed in cold water and sun-dried, which were then used as weft and created an Ikkat-like effect when woven in the handloom. The bleaching was performed by using 30% (w/v) hydrogen peroxide (6%), sodium silicate (3%), tri-sodium phosphate (2%), sodium carbonate (2%), and detergent (0.5%) at a temperature of 85OC for 2 hours keeping material to liquor ratio 1:30 at pH
10.5-11 followed by hot wash at 70OC and cold wash. After drying, these partially bleached yarns were used as weft to achieve the desired design effect on the fabric. This resist bleaching technique is an entirely new approach to creating value-added jute fabric used in apparel and has not been practised before.
The darkening of the jute fibre on treatment with strong alkali is highly undesirable. But in this invention, this darkened effect is very judiciously used vide masking particular / desired portions for the first time to add prominence to the woven designs. The value-added localised white jute textile structure where selectively bleached jute yarns are used as weft and create a selective resisting effect when woven in the loom. The process of producing yarn tie-dye fabric involves the use of dye and water. The said jute yarns are subjected to removal of hemicellulose and developing crimps caused due to the differential shrinkage of the matrix to make the fibre softer than the raw fibres. The process as mentioned here is sustainable, eco-friendly and cost-effective as it does not require any dyeing and gives the Ikkat-like effect just by the bleaching process. Generally, the process of producing Ikkat fabric involves the usage of dye and water but the process of resisting jute through bleaching can produce similar effects in a single process.
The products made from this process are one of the measures for the upliftment of the traditional handloom sectors of Bengal (especially the Dhokra craft cluster of North Bengal) as they can make diversified products

using this technique and present innovation may help uplift the jute fibre itself as it can be used for making value-added textiles.
Technical Details

Loom Used Primary Dobby Loom
Fabric Width 52 inches
Weave Plain
Warp Yarns Mercerised Cotton
Warp Count 2/100s Ne
Weft Yarns Partially Bleached Jute
Weft Count 8 lb/Spy
Heald Shaft 02
Reed Count 72s Stock Ports
Drafting Order 1 end per heald shaft (both for the selvedge and
the body)
Denting Order 4 ends per 1 dent (for selvedge) and 2 ends per 1
dent (for body)



The foregoing description of exemplary embodiments of the invention has been presented for purposes of illustration and description. It is not intended to be exhaustive or to limit the invention to the precise form disclosed, and modifications and variations are possible in light of the above teachings or may be acquired from the practice of the invention. The functionality described may be implemented in a single executable or application or may be distributed among modules that differ in number and distribution of functionality from those described herein.
, Claims:We Claim:

1) A process for localised whitening of jute through bleaching to create value-added textiles with resisting effect comprising the steps of: providing jute yarns for subjecting them to swelling agents by treating them with 10% (w/v) sodium hydroxide (NaOH) at room temperature for 45 minutes, followed by washing;
placing the alkali-treated jute yarns in creel as per the loom specifications and then tying using plastic sheets / masked to prevent the bleaching agent from going inside the tied portions;
performing bleaching process to the said alkali-treated jute yarns is done with 30% (w/v) hydrogen peroxide (6%), sodium silicate (3%), tri- sodium phosphate (2%), sodium carbonate (2%), and detergent (0.5%) at a temperature of 85O C for 2 hours keeping material to liquor ratio 1:30 at pH 10.5-11 followed by hot wash (70OC); and.
performing washing in cold water and sun-drying.

2) The process as claimed in claim 1 wherein the bleaching of the particular portions of alkali treated jute fibre are masked to add prominence to the woven designs.
3) The process as claimed in claim 1 wherein the said jute yarns are subjected to removal of hemicellulose and developing crimps caused due to the differential shrinkage of the matrix to make the fibre softer than the raw fibres.
4) The process as claimed in claim 1 wherein said jute yarn is bleached at a selective portion and is used as weft and creates a selective resisting effect when woven in the loom.
5) The jute yarn with resisting effect being manufactured by employing the

process as claimed in any of the preceding claims.

(Soumah Mitra) IN/PA -664
For the Applicant

Documents

NameDate
202431031716-COMPLETE SPECIFICATION [22-04-2024(online)].pdf22/04/2024
202431031716-DRAWINGS [22-04-2024(online)].pdf22/04/2024
202431031716-ENDORSEMENT BY INVENTORS [22-04-2024(online)].pdf22/04/2024
202431031716-FORM 1 [22-04-2024(online)].pdf22/04/2024
202431031716-FORM 18 [22-04-2024(online)].pdf22/04/2024
202431031716-FORM 3 [22-04-2024(online)].pdf22/04/2024
202431031716-FORM-9 [22-04-2024(online)].pdf22/04/2024
202431031716-POWER OF AUTHORITY [22-04-2024(online)].pdf22/04/2024
202431031716-REQUEST FOR EARLY PUBLICATION(FORM-9) [22-04-2024(online)].pdf22/04/2024